Problems and Countermeasures of wave soldering (1)
Nov 25, 2019| Shenzhen Shenchuang Hi-tech Electronics Co., Ltd(SChitec) is a high tech enterprise which specialized in phone accessories production and sales. Our main products include travel chargers, car chargers, USB cables, power banks and other digital products.All products are safe and reliable, with unique styles.products pass certificates like CE,FCC,ROHS,UL,PSE,C-Tick,etc, If you are interested in, you can contact ceo@schitec.com directly.
Stay Charging Safely with SChitec
Problems and Countermeasures of wave soldering (1)
Insufficient solder
Preventive measures for causes
PCB preheating and welding temperature are too high, so that the viscosity of molten solder is too low. The preheating temperature is 90-130 ℃, and the upper limit is taken when there are many components to be mounted; the tin wave temperature is 250 ± 5 ℃, and the welding time is 3-5s.
The hole diameter of the inserting hole is too large, and the solder flows out of the hole. The hole diameter of the plug-in hole is 0.15-0.4mm larger than the pin diameter (take the lower limit for fine pin and the upper limit for coarse pin).
Small lead large pad, solder is pulled to the pad, so that the solder joints are dry. The pad design shall meet the requirements of wave soldering.
The quality of metallized hole is poor or flux flows into the hole. Reflect to PCB processing plant, improve processing quality.
The crest height is not enough. It can not make PCB produce pressure on solder, which is not conducive to tin. The peak height is generally controlled at 2 / 3 of the PCB thickness.
The climbing angle of PCB is small, which is not conducive to flux exhaust. PCB climbing angle is 3-7 °
Too much solder
The welding temperature is too low or the conveyor belt speed is too fast, so the viscosity of the molten solder is too high. The temperature of tin wave is 250 ± 5 ℃, and the welding time is 3-5s.
Set preheating temperature according to PCB size, multi-layer board, number of components and whether components are installed.
Poor flux activity or low specific gravity. Change flux or adjust proper specific gravity.
Poor solderability of pad, inserting hole and pin. To improve the processing quality of PCB, components should be used first, not stored in humid environment.
When the proportion of tin in solder decreases or the impurity content in solder is too high (Cu < 0.08%), the viscosity and fluidity of molten solder increase. When the proportion of tin is less than 61.4%, some pure tin can be added properly. When the impurity is too high, the solder should be replaced.
Too much solder residue. Debris shall be removed at the end of each day's work.
Tin wire
The preheating temperature of PCB is too low, because the temperature of PCB and components is too low, the solder splashed out when contacting with wave crest is pasted on the surface of PCB. Increase the preheating temperature or extend the preheating time.
The printed board is damp. Dehumidification of PCB.
The resistance welding film is rough and uneven in thickness. Improve the processing quality of PCB.
Missing welding (faulty welding) < rough, granular, poor gloss, poor fluidity >
Explanation: in general, copper tin alloy layer of appropriate thickness is not formed on the joint boundary during brazing.
Causes of missing (faulty) welding:
1. Insufficient heat supply due to low brazing temperature Solder groove temperature is low - clamping speed is too fast - poor design.
2. Poor solderability of PCB or component lead Oxidation pollution of the joined base metal - too high solder temperature - too low solder temperature - too long welding time.
3. The solder shakes before solidification.
4. Flux is flowing in.
Solution for missing (faulty) welding:
1. Clean all welded surfaces before welding. Ensure weldability.
2. Adjust the welding temperature.
3. Enhance the flux activity.
4. Select welding time reasonably.
5. Improve the storage conditions and shorten the storage time of PCB and components.
Cold welding
Explanation of cold welding terms: after wave soldering, there are irregular fillet welds with surge shape at the solder joints, and there is no wetting or insufficient wetting between the base metal box solders, or even cracks.
Due to the vibration of the conveyor belt, the solder is disordered due to the external force when it is cooled. Check whether the motor is faulty and whether the voltage is stable. Whether the conveyor belt has foreign matters.
The welding temperature is too low or the conveyor belt speed is too fast, so the viscosity of the molten solder is too high. Wrinkle the solder joint surface. The temperature of tin wave is 250 ± 5 ℃, and the welding time is 3-5s. When the temperature is a little low, the conveyor belt should be slowed down.
Causes of cold welding:
1. Solder groove temperature is low.
2. The clamping speed is too high and the welding time is short.
3. During the normal welding of PCB, due to the large heat capacity of the component's pin solder joints, the accumulated heat is not enough.
Cold welding solutions:
1. Raise the solder groove temperature.
2. Reduce the clamping speed and control the welding time within 3-5s.
3. Increase the preheating temperature to reduce the thermal shock of PCB from preheating area to solder groove.